Grade | Preliminary drying | Barrel temperature (℃) | Screw rotation (rpm) | Back pressure (MPa) | Mold temperature (℃) | |||
---|---|---|---|---|---|---|---|---|
Nozzle | C3 | C2 | C1 | |||||
General purpose 020/020SF,050/050SF, 070/070SF,080/080SF |
3 - 5hrs 80 - 85℃ |
210 - 230 | 210 - 230 | 190 - 210 | 170 - 190 | 70 - 90 | 10 - 20 | 40 - 60 |
GF-reinforced GRSJ1 GRSJ, GRS GRSJ3 |
3 - 5hrs 80 - 85℃ |
230 - 250 | 230 - 250 | 210 - 230 | 190 - 210 | 40 - 60 | 10 - 20 | 60 - 80 |
Flame-retardant NF012A, SR20 |
3 - 4hrs 70 - 80℃ |
170 - 190 | 170 - 190 | 160 - 170 | 150 - 160 | 40 - 60 | 5 - 15 | 40 - 60 |
Grade | Preliminary drying | Barrel temperature(℃) | Screw rotation (rpm) | Back pressure (MPa) | Mold temperature (℃) | |||
---|---|---|---|---|---|---|---|---|
Nozzle | C3 | C2 | C1 | |||||
MAS10 / MAS10F MAS30 / MAS30F |
3 - 5hrs 80 - 85℃ |
210 - 230 | 210 - 230 | 190 - 210 | 170 - 190 | 70 - 90 | 10 - 20 | 40 - 60 |
Grade | Preliminary drying | Barrel temperature(℃) | Screw rotation (rpm) | Back pressure (MPa) | Mold temperature (℃) | |||
---|---|---|---|---|---|---|---|---|
Nozzle | C3 | C2 | C1 | |||||
General purpose, Easy flow Transparent 300/300SF, 320/320SF 500/500SF, 510/510SF 520/520SF, 660/660SF 680/680SF, T500/T500SF T550/T550SF, T800/T800SF 650, 860, 910B, MX5 |
3 - 5hrs 80 - 85℃ |
210 - 230 | 210 - 230 | 190 - 210 | 170 - 190 | 70 - 90 | 10 - 20 | 40 - 60 |
Heat resistant 450SF |
3 - 5hrs 80 - 85℃ |
230 - 240 | 230 - 240 | 210 - 220 | 200 - 210 | 70 - 90 | 10 - 20 | 40 - 60 |
Heat resistant 400N, 400T |
3 - 5hrs 80 - 85℃ |
240 - 250 | 240 - 250 | 220 - 230 | 210 - 220 | 70 - 90 | 10 - 20 | 40 - 60 |
Heat resistant 460M, 462M 464MD,466MD |
3 - 5hrs 80 - 90℃ |
240 - 260 | 240 - 260 | 220 - 240 | 200 - 230 | 50 - 100 | 10 - 20 | 40 - 60 |
GF-reinforced VGR10/VGR10F VGR20/VGR20F VGR30/VGR30F |
3 - 5hrs 80 - 85℃ |
230 - 250 | 230 - 250 | 210 - 230 | 190 - 210 | 40 - 60 | 10 - 20 | 60 - 80 |
Grade | Preliminary drying | Barrel temperature(℃) | Screw rotation (rpm) | Back pressure (MPa) | Mold temperature (℃) | |||
---|---|---|---|---|---|---|---|---|
Nozzle | C3 | C2 | C1 | |||||
VF512 | 3 - 4hrs 70 - 80℃ |
185 - 195 | 185 - 195 | 170 - 180 | 160 - 170 | 40 - 60 | 5 - 15 | 40 - 60 |
VF191 | 3 - 4hrs 70 - 80℃ |
220 - 230 | 220 - 230 | 200 - 210 | 180 - 190 | 40 - 60 | 5 - 15 | 40 - 60 |
V790 | 3 - 4hrs 70 - 80℃ |
195 - 205 | 195 - 205 | 185 - 195 | 170 - 180 | 40 - 60 | 5 - 15 | 40 - 60 |
SER20 SER22 | 3 - 4hrs 70 - 80℃ |
190 - 200 | 190 - 200 | 170 - 180 | 160 - 170 | 40 - 60 | 5 - 15 | 40 - 60 |
SER80 | 3 - 4hrs 70 - 80℃ |
210 - 220 | 210 - 220 | 190 - 200 | 170 - 180 | 40 - 60 | 5 - 15 | 40 - 60 |
SER91 SER91X | 3 - 4hrs 70 - 80℃ |
220 - 230 | 220 - 230 | 200 - 210 | 180 - 190 | 40 - 60 | 5 - 15 | 40 - 60 |
SER95 | 3 - 4hrs 70 - 80℃ |
225 - 235 | 225 - 235 | 205 - 215 | 185 - 195 | 40 - 60 | 5 - 15 | 40 - 60 |
SERG1 SERG2 SERG3 | 3 - 4hrs 70 - 80℃ |
200 - 220 | 200 - 220 | 180 - 200 | 160 - 180 | 40 - 60 | 5 - 15 | 60 - 80 |
SERG10 SERG20 SERG30 | 3 - 4hrs 70 - 80℃ |
220 - 240 | 220 - 240 | 200 - 220 | 180 - 200 | 40 - 60 | 10 - 20 | 60 - 80 |
Grade | Preliminary drying | Barrel temperature(℃) | Screw rotation (rpm) | Back pressure (MPa) | Mold temperature (℃) | |||
---|---|---|---|---|---|---|---|---|
Nozzle | C3 | C2 | C1 | |||||
AF800 | 3 - 4hrs 80℃ | 220 - 240 | 220 - 240 | 200 - 220 | 180 - 200 | 40 - 60 | 5 - 15 | 40 - 60 |
*“CELPURGE” is recommendable for purging of CEVIAN.